Hobart Multi-Handler 200 settings chart

Power you plug into
Metal thickness
Hobart Multi-Handler 200From the maker's chart

1/8 in (about 3.2 mm) steel, .030 in wire, on 120 V power

Voltage setting19.0
Wire feed setting352

On the maker's chart. A starting point: run a test bead on scrap first.

Gas: C25 (75% Ar / 25% CO2) at 20–30 CFH · Polarity: DCEP

Starting settings for the Hobart Multi-Handler 200, read from Hobart's own chart in the owner's manual. Change the wire, gas or thickness and the card updates.

Setting it on the machine

  1. Press the process select button to choose MIG, flux-cored, TIG or stick.
  2. MIG and flux-cored: the voltage knob sets the voltage and the wire feed/amperage knob sets the wire feed. Both numbers show on the display. Start from the chart numbers on this page.
  3. Stick and TIG: the wire feed/amperage knob sets the amps.

From: Owner's manual section 5-1 (controls, printed page 27) and the process pages that follow (printed pages 28 to 34).

The full chart

Hobart's chart, redrawn so it fits a phone. Thickness runs down the side and wire size across the top.

Steel: Solid ER70S-6, C25 (75% Ar / 25% CO2)

Gas: C25 (75% Ar / 25% CO2), 20–30 CFH · Polarity: DCEP

120 V power. Each cell: voltage setting / wire feed setting.
Thickness.024 in wire.030 in wire.035 in wire
24 ga0.6 mm14.4/13014.0/94–
22 ga0.8 mm14.6/15014.1/109–
20 ga0.9 mm15.2/18515.2/120–
18 ga1.2 mm16.5/25016.1/15715.7/135
16 ga1.5 mm17.8/35017.0/17415.7/155
14 ga1.9 mm19.0/40517.4/24816.6/180
1/8 in3.2 mm21.0/58419.0/35218.3/270
240 V power. Each cell: voltage setting / wire feed setting.
Thickness.024 in wire.030 in wire.035 in wire
24 ga0.6 mm14.3/13714.0/100–
22 ga0.8 mm14.6/16514.1/105–
20 ga0.9 mm15.2/21015.2/120–
18 ga1.2 mm16.3/30016.1/15715.1/130
16 ga1.5 mm18.0/40017.0/17415.3/154
14 ga1.9 mm19.3/46017.4/24816.4/160
1/8 in3.2 mm20.3/49418.5/31817.5/246
3/16 in4.8 mm22.0/65020.8/42018.5/280
1/4 in6.4 mm22.3/65021.7/48619.0/305
5/16 in7.9 mm–23.0/53520.0/360
3/8 in9.5 mm–23.7/60020.5/375
Steel: Solid ER70S-6, 100% CO2

Gas: 100% CO2, 20–30 CFH · Polarity: DCEP

120 V power. Each cell: voltage setting / wire feed setting.
Thickness.024 in wire.030 in wire.035 in wire
18 ga1.2 mm18.0/230––
16 ga1.5 mm19.5/34917.7/18317.4/142
14 ga1.9 mm20.2/44019.3/21518.4/185
1/8 in3.2 mm20.7/48021.0/26019.8/226
240 V power. Each cell: voltage setting / wire feed setting.
Thickness.024 in wire.030 in wire.035 in wire
18 ga1.2 mm17.3/23017.2/14917.0/113
16 ga1.5 mm17.6/23917.7/18317.2/146
14 ga1.9 mm18.2/37819.3/21518.4/170
1/8 in3.2 mm22.3/55520.2/29019.3/241
3/16 in4.8 mm24.7/65021.9/36821.0/290
1/4 in6.4 mm–22.6/38121.7/330
5/16 in7.9 mm–23.0/47524.0/412
3/8 in9.5 mm–25.7/53024.0/418
Stainless steel: Stainless 308L, 98% Ar / 2% CO2

Gas: 98% Ar / 2% CO2, 20–30 CFH · Polarity: DCEP

120 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire
18 ga1.2 mm15.2/242
16 ga1.5 mm16.0/264
14 ga1.9 mm18.0/334
1/8 in3.2 mm19.2/400
240 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire.035 in wire
18 ga1.2 mm15.3/242–
16 ga1.5 mm16.6/29515.5/235
14 ga1.9 mm17.3/37016.2/265
1/8 in3.2 mm18.3/41018.8/355
3/16 in4.8 mm20.2/50519.5/415
1/4 in6.4 mm24.0/50524.6/440
5/16 in7.9 mm24.8/56025.0/450
3/8 in9.5 mm25.6/58025.1/455
Steel: Flux-cored E71T-11, no gas

No shielding gas · Polarity: DCEN

120 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire.035 in wire
18 ga1.2 mm13.1/14013.3/108
16 ga1.5 mm14.2/16013.5/114
14 ga1.9 mm17.5/26416.3/175
1/8 in3.2 mm19.8/31118.5/189
3/16 in4.8 mm21.0/35619.3/210
240 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire.035 in wire.045 in wire
18 ga1.2 mm13.1/14014.0/94–
16 ga1.5 mm16.5/23515.0/11014.0/90
14 ga1.9 mm17.5/30616.0/13014.2/112
1/8 in3.2 mm19.8/36218.5/18914.9/137
3/16 in4.8 mm20.7/39520.4/23819.0/170
1/4 in6.4 mm21.1/40421.7/27519.6/200
5/16 in7.9 mm–23.2/30020.0/205
3/8 in9.5 mm–23.4/37020.1/220
Aluminum (optional SpoolRunner 100 spool gun): 4043, 100% Argon

Gas: 100% Argon, 20–30 CFH · Polarity: DCEP

120 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire
18 ga1.2 mm14.2/304
16 ga1.5 mm14.9/309
14 ga1.9 mm15.6/345
1/8 in3.2 mm19.3/405
240 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire.035 in wire
18 ga1.2 mm13.0/230–
16 ga1.5 mm14.9/309–
14 ga1.9 mm16.0/355–
1/8 in3.2 mm19.3/42219.4/346
3/16 in4.8 mm23.0/52522.2/414
Aluminum (optional SpoolRunner 100 spool gun): 5356, 100% Argon

Gas: 100% Argon, 20–30 CFH · Polarity: DCEP

120 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire
18 ga1.2 mm13.6/330
16 ga1.5 mm14.3/350
14 ga1.9 mm17.4/463
1/8 in3.2 mm20.2/650
240 V power. Each cell: voltage setting / wire feed setting.
Thickness.030 in wire.035 in wire
18 ga1.2 mm13.6/330–
16 ga1.5 mm14.3/350–
14 ga1.9 mm17.4/463–
1/8 in3.2 mm20.2/65019.5/485
3/16 in4.8 mm–21.0/650

TIG welding (DC, steel and stainless)

DCEN polarity, 100% argon at 20-30 CFH. The wire feed/amperage knob sets the amps. The chart gives the same amps on 120 V and 240 V, and adds 1/4 in on 240 V with a 3/32 in tungsten.

Amps, by metal thickness. Source: Welding Parameter Charts, sections 5-12 and 5-13, TIG block.
Thickness1/16 in tungsten3/32 in tungsten
24 gauge2727
22 gauge3030
20 gauge3535
18 gauge5050
16 gauge6060
14 gauge7575
1/8 in125125
3/16 in137137
1/4 in (240 V only)–175

Stick welding on 120 V

Steel. The wire feed/amperage knob sets the amps. The chart gives no 120 V settings for 5/32 in electrodes. Check the chart in the manual for the polarity of your electrode.

Amps, by metal thickness. Source: Welding Parameter Chart - 120V, section 5-12, Stick block.
Electrode16 gauge14 gauge1/8 in3/16 in1/4 in
6011, 3/32 in40456085–
6011, 1/8 in–60758595
6013, 3/32 in45657085–
6013, 1/8 in–60859095
7014, 3/32 in60708590–
7014, 1/8 in60708590100
7018, 3/32 in60708590–
7018, 1/8 in––9095–

Stick welding on 240 V

Steel. The wire feed/amperage knob sets the amps. Thicker electrodes and thicker metal are listed on 240 V only.

Amps, by metal thickness. Source: Welding Parameter Chart - 240V, section 5-13, Stick block.
Electrode16 ga14 ga1/8 in3/16 in1/4 in5/16 in3/8 in
6011, 3/32 in42456085–––
6011, 1/8 in–608090100110–
6011, 5/32 in––125130145150–
6013, 3/32 in45657090–––
6013, 1/8 in–608095115130155
6013, 5/32 in––120130150155160
7014, 3/32 in50708595–––
7014, 1/8 in––100110125135140
7014, 5/32 in––115120145150155
7018, 3/32 in65708595–––
7018, 1/8 in––105115120130135
7018, 5/32 in––115120140145160

What the manual says about this chart

  • Cells are 'voltage setting / wire feed setting', as shown on the welder's display.
  • Two charts: 120 V (24 gauge to 3/16 in; the 1/4 in column is blank for every wire) and 240 V (24 gauge to 3/8 in).
  • The chart marks blank cells as 'not recommended'.
  • Chart says: settings are approximate; thicker materials can be welded with proper technique, joint preparation and multiple passes; suggested gas flow 20-30 cfh.
  • Aluminum settings are with the optional SpoolRunner 100 spool gun.
  • Rated MIG output from the manual's specifications: 200 A at 24 V, 15% duty cycle on 240 V; 100 A at 19 V, 40% duty cycle on 120 V.

Source

Hobart Multi-Handler 200 owner's manual OM-285922C. Sections 5-12 (120 V chart, printed page 38, PDF page 42) and 5-13 (240 V chart, printed page 39, PDF page 43).

Read on 2026-11-26. Status: read from the manual, waiting for a welding inspector's check. We link to the manual and do not copy its pages. How we check numbers. Spotted a mistake? Tell us.