Pre-launch draft. Numbers await a welding inspector's check.

Hobart IronMan 240 settings chart

Metal thickness
Hobart IronMan 240From the maker's chart

1/8 in (about 3.2 mm) steel, .030 in wire

11010100
Voltage knob2.5 of 10
Wire feed knob30

On the maker's chart. A starting point: run a test bead on scrap first.

Gas: 75% Ar + 25% CO2 · Polarity: DCEP

Starting settings for the Hobart IronMan 240, read from Hobart's own chart in the owner's manual. Change the wire, gas or thickness and the card updates.

Setting it on the machine

  1. The voltage control is a knob marked 1 to 10. Turn it clockwise for more voltage.
  2. The wire feed control is a knob marked 10 to 100. Turn it clockwise for more wire feed speed.
  3. These are knob numbers, not real volts or inches per minute, so they only match this welder's own chart.
  4. The welder shuts the weld output off if no arc starts within 3 seconds of pulling the trigger, and if the contact tip shorts to the work.

From: Owner's manual section 6-1 (controls, printed page 26).

The full chart

Hobart's chart, redrawn so it fits a phone. Thickness runs down the side and wire size across the top.

Steel: Solid ER70S-6, 75% Ar + 25% CO2

Gas: 75% Ar + 25% CO2 · Polarity: DCEP

Each cell: voltage knob / wire feed knob.
Thickness.024 in wire.030 in wire.035 in wire.045 in wire
24 ga0.6 mm1.1/200.8/15––
22 ga0.8 mm1.8/281/15––
18 ga1.2 mm1.9/351/201.2/20–
16 ga1.5 mm2/401.5/202/201.5/20
14 ga1.9 mm4.5/802/252/251.9/22
1/8 in3.2 mm–2.5/302.6/352.3/25
3/16 in4.8 mm–2.8/353/402.5/25
1/4 in6.4 mm–4/504.2/504/30
3/8 in9.5 mm–5/607.5/558.5/45
1/2 in12.7 mm–––9/50

Steel: Solid ER70S-6, 100% CO2

Gas: 100% CO2 · Polarity: DCEP

Each cell: voltage knob / wire feed knob.
Thickness.024 in wire.030 in wire.035 in wire.045 in wire
24 ga0.6 mm2.3/15–––
22 ga0.8 mm3/21–––
18 ga1.2 mm3.4/281.5/151.5/17–
16 ga1.5 mm3.9/402.5/182.1/211.7/13
14 ga1.9 mm4.5/532.8/253.1/222.5/20
1/8 in3.2 mm5.1/703.2/353.5/223.3/22
3/16 in4.8 mm5.6/754/404.1/314/28
1/4 in6.4 mm–4.5/455/404.3/29
3/8 in9.5 mm–7.5/656.6/496.5/36
1/2 in12.7 mm–––7.3/45

Steel: Flux-cored E71T-11, no gas

No shielding gas · Polarity: DCEN

Each cell: voltage knob / wire feed knob.
Thickness.030 in wire.035 in wire.045 in wire
18 ga1.2 mm1/22––
16 ga1.5 mm1.3/261.5/15–
14 ga1.9 mm2/352/170.9/14
1/8 in3.2 mm3.2/353.5/231.8/14
3/16 in4.8 mm4/414/303.2/21
1/4 in6.4 mm5/535.5/403.6/28
3/8 in9.5 mm–6/505/38
1/2 in12.7 mm––7.8/41

Steel: Solid ER70S-6, 90% Ar / 10% CO2

Gas: 90% Ar / 10% CO2 · Polarity: DCEP

Each cell: voltage knob / wire feed knob.
Thickness.030 in wire.035 in wire.045 in wire
24 ga0.6 mm0/15––
22 ga0.8 mm0/18––
18 ga1.2 mm1/200.8/18–
16 ga1.5 mm1/252/301.7/21
14 ga1.9 mm1.5/302.5/352.2/21
1/8 in3.2 mm2.7/403/402.4/28
3/16 in4.8 mm3.2/504/423/28
1/4 in6.4 mm4/554.5/507.2/40
3/8 in9.5 mm5/708/657.5/43
1/2 in12.7 mm––8/45

Stainless steel: Stainless ER308 / 308L / 308LSi, 98% Ar / 2% CO2

Gas: 98% Ar / 2% CO2 · Polarity: DCEP

Each cell: voltage knob / wire feed knob.
Thickness.030 in wire.035 in wire
22 ga0.8 mm1/220/17
18 ga1.2 mm1.5/311/20
16 ga1.5 mm2/381.5/29
14 ga1.9 mm2.2/451.9/32
1/8 in3.2 mm3.3/602.4/39
3/16 in4.8 mm4.5/652.9/45
1/4 in6.4 mm7/707/50
3/8 in9.5 mm8/808.6/70

Aluminum (SpoolRunner 200 spool gun): ER4043, 100% Argon

Gas: 100% Argon · Polarity: DCEP

Each cell: voltage knob / wire feed knob.
Thickness.030 in wire.035 in wire.047 in wire
16 ga1.5 mm0.9/510/32–
14 ga1.9 mm1.9/541/42–
1/8 in3.2 mm4.5/604.6/45–
3/16 in4.8 mm6.5/756/605.9/40
1/4 in6.4 mm7.1/877.5/757/48
3/8 in9.5 mm–8/858.3/50
1/2 in12.7 mm––8.6/54

Aluminum (SpoolRunner 200 spool gun): ER5356, 100% Argon

Gas: 100% Argon · Polarity: DCEP

Each cell: voltage knob / wire feed knob.
Thickness.035 in wire.047 in wire
16 ga1.5 mm0.1/61–
14 ga1.9 mm0.7/70–
1/8 in3.2 mm4.8/903.9/41
3/16 in4.8 mm–5/54
1/4 in6.4 mm–6.9/70

What the manual says about this chart

  • Cells are 'voltage knob setting / wire feed knob setting'.
  • The chart runs from 24 gauge to 1/2 in. It has no 20 gauge column and no 5/16 in column.
  • Some voltage settings on the chart are below the first mark on the knob, such as 0, 0.1 and 0.8. They are shown here as printed.
  • Self-shielded flux-cored wire (E71T-11) is the only row on DCEN polarity. Every other row is DCEP.
  • Aluminum settings are with the SpoolRunner 200 spool gun and 100% argon.
  • Rated output from the manual's specifications: 280 A at 28.2 V, 30% duty cycle. Amperage range 30 to 280 A. This welder needs a 208 or 240 V supply, with its jumper links set to match.

Source

Hobart IronMan 240 owner's manual OM-284833G. Section 5-13, Weld Parameters, printed pages 24 and 25 (PDF pages 28 and 29).

Read on 2026-11-26. Status: read from the manual, waiting for a welding inspector's check. We link to the manual and do not copy its pages. How we check numbers. Spotted a mistake? Tell us.

Other welders

Open the settings tool for any welder

Settings right but the weld still looks wrong?

Pinholes, spatter, holes in thin metal or a bead that sits on top each have their own fix. Fix a bad MIG weld