Forney 220 MP settings chart
1/8 in (about 3.2 mm) steel, .030 in wire
On the maker's chart. A starting point: run a test bead on scrap first.
Gas: C25 (75% Ar / 25% CO2) · Polarity: DCEP
Starting settings for the Forney 220 MP, read from Forney's own chart in the owner's manual. Change the wire, gas or thickness and the card updates.
Setting it on the machine
- Press the process selector button to the top position for MIG or flux-cored welding.
- The left knob sets arc voltage and the right knob sets wire feed speed in inches per minute. Start in the middle of the chart's range and adjust from there.
- Polarity is set with the jumper lead: for gasless flux-cored wire, jumper to negative and ground cable to positive; for MIG with gas, jumper to positive and ground cable to negative.
- The manual gives the knob ranges as 13 to 25 volts and 90 to 550 IPM on 230 V, and 13 to 20 volts and 90 to 220 IPM on 120 V. Chart settings above those limits need 230 V.
From: Owner's manual pages 12 and 13 (controls) and page 19 (MIG and flux-cored set-up).
The full chart
Forney's chart, redrawn so it fits a phone. Thickness runs down the side and wire size across the top.
Steel: Solid ER70S-6, C25 (75% Ar / 25% CO2)
Gas: C25 (75% Ar / 25% CO2) · Polarity: DCEP
| Thickness | .030 in wire | .035 in wire |
|---|---|---|
| 18 ga1.2 mm | 16–17/ | 16–17/ |
| 16 ga1.5 mm | 17–18/ | 17–18/ |
| 14 ga1.9 mm | 17–18/ | 17–18/ |
| 1/8 in3.2 mm | 17.5–19/ | 18–19/ |
| 3/16 in4.8 mm | 18–19/ | 18–19/ |
| 1/4 in6.4 mm | – | 21–22/ |
| 5/16 in7.9 mm | – | 21–22/ |
| 3/8 in9.5 mm | – | 23–24/ |
Steel: Flux-cored E71T-GS, no gas
No shielding gas · Polarity: DCEN
| Thickness | .030 in wire | .035 in wire |
|---|---|---|
| 14 ga1.9 mm | 14–15/ | 14–15/ |
| 1/8 in3.2 mm | 14–15/ | 14–15/ |
| 3/16 in4.8 mm | 15–16/ | 15–16/ |
| 1/4 in6.4 mm | – | 15–16/ |
| 5/16 in7.9 mm | – | 16–17/ |
| 3/8 in9.5 mm | – | 16–17/ |
Aluminum (spool gun): ER4043, 100% Argon
Gas: 100% Argon · Polarity: DCEP
| Thickness | .030 in wire | .035 in wire |
|---|---|---|
| 16 ga1.5 mm | 14–16/ | – |
| 14 ga1.9 mm | 15–17/ | 14–16/ |
| 1/8 in3.2 mm | 22–24/ | 21–22/ |
| 3/16 in4.8 mm | 24–26/ | 23–24/ |
| 1/4 in6.4 mm | – | 24–25/ |
Stick welding
The left knob sets the amps. The chart gives a range of amps for each electrode diameter, not for each metal thickness, with the polarity each electrode type can run on. This welder's output is DC only.
| Electrode | 1/16 in (1.6 mm) | 3/32 in (2.4 mm) | 1/8 in (3.2 mm) | 5/32 in (4.0 mm) |
|---|---|---|---|---|
| E6010 (DCEP) | – | 30–75 | 75–125 | 110–165 |
| E6011 (AC, DCEP) | – | 40–85 | 75–125 | 110–165 |
| E6013 (AC, DCEP, DCEN) | 20–45 | 40–90 | 70–110 | 115–140 |
| E7014 (AC, DCEP, DCEN) | – | 70–90 | 90–140 | 140–190 |
| E7018 (DCEP) | – | 65–100 | 110–165 | 150–220 |
| E308L / E309L / E316L stainless (DCEP) | 20–40 | 40–70 | 75–115 | 105–160 |
Stick welding amperage chart: these amps next to other makers' charts
TIG welding (DC, lift arc)
DCEN polarity, 100% argon. The left knob sets the amps. The chart lists a 3/8 in (#6) gas cup, or 7/16 in (#7) for 3/16 in metal. The manual recommends lanthanated tungsten in its text and 2% ceriated tungsten on the chart.
| Metal thickness | Amps | Filler rod | Tungsten |
|---|---|---|---|
| 1/16 in | 50–80 | 1/16 in | 1/16 in |
| 3/32 in | 80–110 | 1/16 in | 1/16 in |
| 1/8 in | 85–120 | 3/32 in | 1/16 in |
| 3/16 in | 125–200 | 1/8 in | 3/32 in |
What the manual says about this chart
- Cells are 'volts / wire feed speed in IPM'. The chart heads the two columns with a V symbol and a wire-feed symbol, and every cell is a range.
- One chart covers both 120 V and 230 V. It does not say which rows need 230 V; the manual's knob limits on 120 V (20 volts, 220 IPM) are below many of the chart's settings.
- The chart starts at 18 gauge and ends at 3/8 in. The .030 wire rows stop at 3/16 in.
- The steel rows are for ER70S-6 solid wire with 75% argon / 25% CO2, and E71T-GS flux-cored wire with no gas.
- Forney's 190 MP and 250 MP PRO charts share most of these solid-wire numbers; each welder's page shows what its own manual prints.
- Aluminum (ER4043, argon) needs a spool gun; the chart says so under the table. The .035 aluminum row lists a lower wire speed at 1/4 in (350–375) than at 3/16 in (430–450). Recorded as printed.
- The manual gives no duty cycle numbers in its text; it points to the data plate on the welder.
Source
Forney 220 MP (item 410) operating manual, rev. 08.08.2019. '220 MP MIG Set-Up Chart', page 19; stick chart, page 20; TIG chart, page 21.
Read on 2026-11-26. Status: read from the manual, waiting for a welding inspector's check. We link to the manual and do not copy its pages. How we check numbers. Spotted a mistake? Tell us.